IS 800:2007

Table of structural steel grades and design strengths (IS 2062 / IS 800)

Yield stress by thickness, ultimate tensile stress and design strengths fy/γm0 and fu/γm1 for IS 2062:2011 grades E250 to E650, with the elastic constants of IS 800.

References:cl. 2.2.4Table 1Table 5IS 2062 Table 2
Report details
IS 2062:2011 hot rolled structural steel
Gradefu (MPa)fy t<20 (MPa)fy 20–40 (MPa)fy >40 (MPa)Elongation (%)fy/γm0 t<20fu/γm1ε (t<20)
E25041025024023023227.3328.01.000
E27543027526525522250.0344.00.953
E30044030029028022272.7352.00.913
E35049035033032022318.2392.00.845
E41054041039038020372.7432.00.781
E45057045043042020409.1456.00.745
E55065055053052012500.0520.00.674
E60073060058057012545.5584.00.645
E65078065063062012590.9624.00.620

Values per IS 2062:2011 Table 2. Confirm the yield stress band for the actual product thickness and supplier certificates.

Detailed calculation

Material constants

2
E=200×103 MPa,G=76.9×103 MPa,ν=0.3E = 200 \times 10^3\ \mathrm{MPa},\quad G = 76.9\times 10^3\ \mathrm{MPa},\quad \nu = 0.3
2.2.4.1
γm0=1.10 (yielding),γm1=1.25 (ultimate),ε=250/fy\gamma_{m0} = 1.10\ (\text{yielding}),\quad \gamma_{m1} = 1.25\ (\text{ultimate}),\quad \varepsilon = \sqrt{250/f_y}
Table 5, Table 2