Hardened concrete — strength tests

Split tensile strength

Indirect tensile strength of concrete on cylinders — used in design studies and for fibre-reinforced or special concretes.

Standards:IS 516 (Part 1/Sec 1):2021 (supersedes IS 5816)

Equipment

  • Cylinder moulds 150 mm dia. × 300 mm
  • Compression machine with a jig and plywood bearing strips (3 mm thick, 25 mm wide)

Procedure

  1. Mark diametral lines on both ends of the cylinder to align it in the jig.
  2. Place the cylinder horizontally between the platens with bearing strips top and bottom.
  3. Load continuously at a rate of 1.2–2.4 N/mm² per minute (splitting stress) until failure.

Calculation

fct=2Pπ l df_{ct} = \dfrac{2P}{\pi\,l\,d}

Results and acceptance criteria

  • Split tensile strength is typically 8–12% of compressive strength.

This page summarises the procedure for site and laboratory use. Follow the current edition of the cited standards (with amendments) and the project specification, which govern.