Rebound hammer test (Schmidt hammer)
Measures surface hardness to assess the uniformity of concrete and, with a site calibration, to estimate compressive strength.
Standards:IS 516 (Part 5/Sec 4):2020 (supersedes IS 13311 Part 2)IS 516 (Part 5/Sec 1) — combined use with UPV
Equipment
- Rebound hammer (type N, impact energy 2.207 N·m) with test anvil for calibration
- Carborundum stone for surface preparation
- Chalk/grid template, data sheet
Procedure
- Check the hammer on its calibration anvil before and after use.
- Select test areas on smooth, dry, formed surfaces at least 25 mm from edges; grind off plaster, laitance and loose material.
- Hold the hammer perpendicular to the surface and press until the plunger releases; read the rebound number. Take about 10–12 readings per test area at points at least 25 mm apart, not on the same spot twice.
- Note the hammer orientation (horizontal, upward, downward) and apply the manufacturer's correction where needed.
- Use the median or mean after discarding abnormal readings; estimate strength only from a correlation established with cores or cubes of the same concrete.
Results and acceptance criteria
- Rebound number reflects only the outer 30–50 mm; carbonation, moisture, surface finish and aggregate type all affect it.
- The rebound estimate of in-situ strength is considered valid only when the UPV indicates good quality concrete (velocity ≥ 3.5 km/s for grades up to M25, ≥ 3.75 km/s above M25) — see the UPV test.
- Accuracy of strength estimates from rebound alone is no better than about ±25%.
This page summarises the procedure for site and laboratory use. Follow the current edition of the cited standards (with amendments) and the project specification, which govern.