Half-cell potential (corrosion probability)
Maps the electrochemical potential of reinforcement to locate areas where corrosion is likely to be active.
Standards:ASTM C876
Equipment
- Copper/copper sulphate (CSE) reference electrode
- High-impedance digital voltmeter (≥ 10 MΩ)
- Connecting leads and clamp for the reinforcement
- Sponge and wetting solution
- Cover meter, drill
Procedure
- Locate the reinforcement with a cover meter; expose a bar and check electrical continuity across the test area.
- Connect the voltmeter positive terminal to the reinforcement and the negative to the electrode.
- Pre-wet the surface, then take readings on a grid (typically 0.5–1.0 m spacing) with the electrode on a wet sponge.
- Plot equipotential contours of the readings.
Results and acceptance criteria
- More positive than −200 mV (CSE): greater than 90% probability of no corrosion.
- −200 to −350 mV: corrosion activity uncertain.
- More negative than −350 mV: greater than 90% probability of active corrosion.
- Readings are influenced by moisture, coatings and carbonation; confirm with breakouts.
This page summarises the procedure for site and laboratory use. Follow the current edition of the cited standards (with amendments) and the project specification, which govern.