Durability and corrosion assessment

Carbonation depth (phenolphthalein test)

Determines how deep the concrete has carbonated. Once carbonation reaches the reinforcement, the protective alkalinity is lost and corrosion can start.

Standards:EN 14630 (method)IS 456 cl. 8 — durability and cover

Equipment

  • 1% phenolphthalein solution in alcohol (spray bottle)
  • Hammer and chisel or core / drill
  • Measuring scale or vernier
  • Brush or blower

Procedure

  1. Expose a freshly broken or freshly cut concrete surface (breakout, core, or split core) — do not use a sawn wet surface without drying.
  2. Remove dust and spray the indicator immediately.
  3. Measure the depth from the surface to the boundary of the pink (magenta) region at several points; report the mean and maximum.

Results and acceptance criteria

  • Pink = alkaline, pH above about 9 (not carbonated); colourless = carbonated.
  • If the carbonation depth approaches or exceeds the cover, reinforcement is at risk of corrosion — check with half-cell potential.

This page summarises the procedure for site and laboratory use. Follow the current edition of the cited standards (with amendments) and the project specification, which govern.