Durability and corrosion assessment

Chloride content of hardened concrete

Measures chloride ions, which destroy the passive film on reinforcement and cause pitting corrosion.

Standards:IS 14959 (Part 2) — hardened concreteIS 456 cl. 8.2.5.2 and Table 7 — limits

Equipment

  • Rotary hammer drill with depth stop (powder sampling at increments)
  • Sample bags
  • Laboratory titration (Volhard / potentiometric) or field chloride kit

Procedure

  1. Drill powder samples at depth increments (e.g. 0–25, 25–50, 50–75 mm), discarding the first few millimetres.
  2. Dissolve in nitric acid (acid-soluble) or water (water-soluble) and titrate for chloride.
  3. Express the result as % by mass of cement or kg/m³ of concrete and plot the chloride profile against depth.

Results and acceptance criteria

  • IS 456 Table 7 (total acid-soluble chloride, kg/m³ of concrete): prestressed concrete 0.4; reinforced concrete or plain concrete with embedded metal 0.6; concrete without embedded metal 3.0.
  • Chloride at the depth of the reinforcement above about 0.4% by mass of cement indicates a significant corrosion risk.

This page summarises the procedure for site and laboratory use. Follow the current edition of the cited standards (with amendments) and the project specification, which govern.