Density checks batching and yield; air content controls durability of air-entrained concrete; temperature controls workability loss and thermal cracking.
Standards:IS 1199 (Part 3):2018 — densityIS 1199 (Part 4):2018 — air content (pressure method)IS 7861 (Part 1) — hot weather concreting
Equipment
- Calibrated rigid container of known volume, balance, tamping rod or vibrator
- Air entrainment meter (pressure type)
- Digital probe thermometer
Procedure
- Density: fill and fully compact the container in layers, strike off, clean and weigh. Density = mass of concrete / volume of container.
- Air content: fill and compact the base of the air meter, clamp the cover, pump to the initial pressure and release; read the air content directly from the gauge. Apply the aggregate correction factor.
- Temperature: insert the thermometer at least 75 mm into the concrete for 2 minutes or until stable.
Calculation
Results and acceptance criteria
- Normal-weight concrete density is typically 2350–2500 kg/m³.
- IS 7861 (Part 1) recommends that the temperature of concrete as placed does not exceed 40 °C; many projects specify 32–35 °C for large pours.
This page summarises the procedure for site and laboratory use. Follow the current edition of the cited standards (with amendments) and the project specification, which govern.