Self-compacting concrete — slump flow, T500, V-funnel, L-box, J-ring
Characterises filling ability, passing ability and segregation resistance of self-compacting concrete (SCC).
Standards:IS 1199 (Part 6):2018IS 10262:2019 (SCC mix design annex)EFNARC guidelines
Equipment
- Slump cone and 1 m × 1 m flat base plate marked with a 500 mm circle
- V-funnel with trap door
- L-box with removable gate and reinforcing bars
- J-ring
- Stopwatch, tape
Procedure
- Slump flow: fill the cone without rodding, lift it, and measure the final spread diameter in two directions; record T500, the time to reach the 500 mm circle.
- V-funnel: fill the funnel, open the gate after 10 s and record the time for all concrete to flow out.
- L-box: fill the vertical section, open the gate, and measure the heights H₁ (behind the gate) and H₂ (at the end) after flow stops.
- J-ring: perform the slump flow test with the J-ring around the cone and compare the spread and the step height with the unrestricted flow.
Calculation
Results and acceptance criteria
- Typical classes (EFNARC): slump flow SF1 550–650 mm, SF2 660–750 mm, SF3 760–850 mm; T500 2–5 s; V-funnel 6–12 s; L-box ratio ≥ 0.8.
This page summarises the procedure for site and laboratory use. Follow the current edition of the cited standards (with amendments) and the project specification, which govern.