Reinforcement — tensile, bend/rebend and mass tests
Confirms the grade, ductility and mass per metre of high strength deformed (TMT) bars.
Standards:IS 1786 — requirementsIS 1608 (Part 1) — tensile testingIS 1599 — bend test
Equipment
- Universal testing machine (UTM) with extensometer
- Bend/rebend mandrels
- Weighing balance and measuring tape
- Vernier caliper
Procedure
- Cut samples from each lot and diameter (length about 0.5–1 m for tensile tests).
- Mass test: weigh a measured length and compare the mass per metre with the nominal value (φ²/162 kg/m).
- Tensile test: mark the gauge length (5.65√A), load in the UTM, record 0.2% proof stress (yield), ultimate tensile strength and elongation after fracture.
- Bend test: bend the bar through 180° over the specified mandrel; rebend test: bend 135°, age, then straighten by 157.5°. Inspect for cracks.
Results and acceptance criteria
- Fe 500: 0.2% proof stress ≥ 500 MPa, tensile strength ≥ 1.08 × proof stress and ≥ 545 MPa, elongation ≥ 12%. Fe 500D: TS/YS ≥ 1.10, TS ≥ 565 MPa, elongation ≥ 16% (IS 1786).
- Mass per metre tolerance (IS 1786): ±7% for bars below 10 mm, ±5% for 10–16 mm, ±3% above 16 mm.
- No transverse cracks after the bend and rebend tests.
This page summarises the procedure for site and laboratory use. Follow the current edition of the cited standards (with amendments) and the project specification, which govern.